Hardness in Spare Parts and Tooling: How to Specify It on the Drawing and Verify It at Receiving

“Hardened” is not a specification. What the hardness callout for a spare part or tooling component has to say (value with a range, scale, test location and, where it applies, case depth), why a conversion between scales can't be used to accept a part, and what to check when it arrives.

The drawing says “hardened” or “hardness 58–62.” The pin arrives, looks fine, gets installed, and a few weeks later it has a wear lip where the part seats. Quality asks for the certificate: it says “58–62 HRC,” the same text as the drawing, with no word on where it was tested or which lot. Or it shows a Brinell value that someone converted to HRC with a chart. Did the part comply? Nobody can say, because nobody wrote down what complying meant.

This guide is for whoever orders or receives hardened spare parts and tooling at a plant: locating pins, bushings, wear plates, gripper fingers, fixture components. It answers two specific questions: what the hardness callout on the drawing or purchase order has to say, and how to verify at receiving that the part complies. It is not a guide to choosing or buying a hardness tester.

In Summary

  • “Hardened” or “high hardness” is not a specification. Without a value with a range, a scale and a test location, there is no criterion to accept or reject the part.
  • A complete callout has five parts: range (minimum and maximum), scale and test standard, test location, case depth if the treatment is surface hardening, and the evidence the supplier delivers.
  • A conversion between scales is an estimate, not a result. ASTM E140 recommends avoiding the conversion of test data whenever possible: if the drawing calls for HRC, acceptance is based on a test in HRC.
  • At receiving, check that the certificate shows the measured hardness, not the drawing value copied over, in the specified scale, with the test location and the lot. If not, the part doesn't get installed yet.
  • With Radii for tooling and MRO, the hardness callout and the evidence you need go into the quote request, together with the drawing.

1. Why “hardened” is not a specification

Hardness is one of the few properties of a spare part you can't see or check with a caliper. A soft part and a hardened one look the same, are machined to the same dimension and pass the same dimensional inspection. The difference shows up later, as wear, deformation or a lip on the diameter of a pin.

That's why the hardness callout isn't a detail on the drawing: it's the only criterion you'll have to file a claim. And an incomplete callout can't be claimed against:

What the drawing saysWhat happens when the part arrivesWhat's missing
“Hardened”Any treatment that hardens the part meets the textValue, range, scale and location
“Hardness 58–62”Nobody knows if it's HRC, HV or HBScale and range
“58 HRC min.”A part that is too hard and brittle also compliesMaximum
“58–62 HRC”The supplier can test wherever, even on a functional faceTest location and evidence
“Nitrided, range in HRC”The surface complies, but nobody knows how much hardened material there isCase depth and method

Which steel and which hardness suit each part is not the subject of this article: for locating pins it's in what material, tolerance and heat treatment fixture pins need. The subject here is how to write the value you already chose so that it can be verified.

2. Which scale to call for

A hardness value without a scale is not a number. Each method tests with a different indenter and force, so each scale works best on a certain kind of part. This table is common industry practice, not a rule from a standard:

ScaleHow it's writtenCommon use
Rockwell CHRCHardened steel: pins, bushings, wear plates, fixture parts
Rockwell BHRBSoft or annealed steel, and nonferrous metals
Rockwell superficialHR + scaleThin cases, small or thin-walled parts
VickersHVThin cases, small parts and testing at specific spots
BrinellHBRaw or annealed bar, and large sections
Leeb (portable, rebound)HL, e.g. HLDLarge parts that don't fit in a benchtop tester

Two clarifications that prevent misunderstandings:

  • Rockwell and Rockwell superficial are the same family. ASTM E18 covers both for metallic materials, with requirements for the machines and for the procedure. According to its scope, the difference between the two is the preliminary (minor) test force.
  • The part decides the scale, not habit. A thin nitrided case tested in HRC can give a reading that doesn't represent it. Leeb is practical on large parts, but its result usually ends up converted, with the limits in section 5. If the treatment is surface hardening, agree on the scale with whoever will do it.

For a hardened spare part or tooling component, HRC is the norm. If your drawing says something else, it should be because the part calls for it.

3. How to write the hardness callout on the drawing or the order

A hardness callout you can verify has five parts. Take this as a format example (not a recommendation for your part): “58–62 HRC · ASTM E18 · test on face A (non-functional) · certificate with measured hardness.”

  1. Value with a range. Minimum and maximum, not a single number. A lone value has no rejection criterion: nobody knows how far below or above it is still acceptable. A minimum with no maximum accepts parts that are too hard and brittle.
  2. Scale and method. The scale the part will be tested in (HRC, HRB, HV, HB) and the test standard; for Rockwell, ASTM E18.
  3. Test location. Where to test: a non-functional face, or a coupon from the same lot and the same treatment. The test leaves an indent, and an indent on the seating face of a locator or on the fit diameter of a pin is a defect you asked for. If core hardness matters for the function, specify it separately.
  4. Case, if surface-hardened. For nitriding, carburizing or induction hardening, the case depth and the method used to determine it (section 4).
  5. Evidence from the supplier. A heat-treat certificate with the measured hardness, the scale, where it was tested and the lot.
Weak calloutComplete callout
“Hardened”Range in HRC · ASTM E18 · face A non-functional · certificate with measured hardness and lot
“Hardness 58–62”Minimum and maximum, with scale (HRC) and test standard
“Harden and grind”Range and test location, plus a note that final dimensions are finished after heat treatment
“Nitride”Surface hardness with range and scale · case depth and test method · area to be treated
“Same as sample”The complete callout, even if you send a sample: the sample doesn't say which scale or where

If the purchase order goes out without a drawing (a spare part replaced using the old one as a reference), the callout still goes on the order. Which documents to ask for with the part, and why you ask before quoting, is covered in quality documentation for a spare part or tooling; here it's enough for the callout to state what hardness evidence you expect.

Anatomy of a hardness callout on the drawing: value with a range, scale and method, test location, case if surface-hardened and evidence from the supplier, with an example callout of 58–62 HRC per ASTM E18

Illustration: Radii conceptual diagram based on ASTM E18 and ISO 18203 (public abstracts). The example range is illustrative, not a recommendation for your part.

4. Through hardening versus surface hardening

Not all hardened parts are the same inside. With through hardening (quenching and tempering the whole part), surface and core hardness depend on the steel and the section, and the callout from section 3 is usually enough. With surface hardening, only a case becomes hard and the core stays softer on purpose: tough inside, wear-resistant outside.

That changes the specification. Surface hardness alone isn't enough, because two parts with the same surface reading can have very different cases underneath. The one with the thinner case wears through to the soft core sooner.

TreatmentWhat you specify besides surface hardnessEvidence you ask for
Through hardening (quench and temper)Test location; core hardness only if it matters for the functionMeasured hardness, scale, location and lot
Induction or flame hardeningCase depth, test method and area to be treatedMeasured surface hardness and case depth
Carburizing (and hardening)Case depth and method; core hardness if it mattersSurface hardness, case depth and, where it applies, core
NitridingCase depth and test methodMeasured surface hardness and case depth

The reference for measuring the case is ISO 18203:2026, Steel — Determination of the thickness of surface-hardened layers. According to its public abstract, it specifies a method for measuring case hardening depth, surface hardening depth, nitriding hardness depth and total thickness of the hardened layer, obtained by thermal treatments (flame, induction, electron beam, laser) or thermochemical treatments (carbonitriding, case hardening, nitriding). Citing it in the callout tells the supplier which method you'll ask the depth to be measured with.

One detail worth writing down: if the part is ground after treatment, the case depth that matters to you is what remains on the finished part. State in the callout whether the depth applies to the finished part, so the supplier leaves enough stock before grinding.

5. Conversions between scales: why they can't be used to accept a part

The drawing calls for HRC, the certificate shows HB or HV (or a Leeb value from a portable tester), and someone runs it through a conversion chart. The number lands inside the range and the part is accepted. The problem is that the acceptance wasn't based on a measurement, but on an estimate.

The standard behind the conversion tables, ASTM E140, says so itself:

  • Conversion is approximate. Going from one scale to another is only an approximate process, because each test measures a different combination of material properties.
  • It depends on the material. Conversions can be affected by alloy, grain structure or heat treatment, among other factors, and are only valid for the materials the standard indicates. Two of its tables cover non-austenitic carbon, alloy and tool steels in the homogeneous condition, and the one relating Leeb D to Brinell, Vickers and Rockwell is for homogeneous non-austenitic steels.
  • Avoid converting results. The standard presents its tables as an estimate and recommends applying them mainly to agreed specification limits, avoiding the conversion of test data whenever possible.
  • Conversion is the last resort. You convert when it is impossible to test the material under the specified conditions.
Use of a conversionDoes it work?Why
Estimating in HRC a value reported in HB or HVYes, as an estimateIt tells you whether to keep checking or whether something is off
Translating a drawing limit to another scale, agreed with the supplierWith prior agreementIt's the use the standard recommends: on limits, not on results
Accepting a part by converting the certificate resultNoIt's an estimate of a test that isn't the one you called for

The practical consequence is simple: if the drawing calls for HRC, ask for the test in HRC. If the part's geometry doesn't allow testing in HRC, the time to solve it is when writing the callout, by changing the scale on the drawing, not at receiving, by converting.

Radii has two free tools for estimating: the HRB and HRC hardness table and the HRC, HRB, HV and HB hardness converter, based on ASTM E140 and the ASM Metals Handbook. They're good for what a conversion is good for: giving you an order of magnitude before asking for the right test. They are not an acceptance criterion.

6. Verifying hardness at receiving

Which certificates to ask for is covered in the quality documentation post linked in section 3; here, how to read the hardness part. Receiving starts with the heat-treat certificate, before any hardness tester. Check four things, in this order:

  1. Does it show measured hardness, not just the drawing value? A certificate that repeats “58–62 HRC” doesn't say what anyone measured. If there's no measured value, ask for it before installing the part.
  2. Is it in the same scale the drawing specifies? If it's in another, a conversion is only an estimate (section 5). Ask for a test in the specified scale.
  3. Does it say where it was tested? A test at one location may not represent the characteristics of the whole part: ASTM E18 says so when describing the use of the test. Without a location, you don't know whether it was tested where it matters or on a face that didn't get the same treatment.
  4. If the drawing calls for a case, does it show the measured depth? If not, ask for the measured case depth and the method used (ISO 18203).

If all four are yes (or not applicable) and the value is inside the range, accept the part and file the certificate with the order.

When to retest? It depends on how critical the part is and on what your plant's quality system requires, since it sets criteria and sampling. Some useful references:

SituationWhat to do
Certificate incomplete or in another scaleAsk the supplier for the right test before installing
Part critical to the line, or a new supplierRetest at the drawing location, in your lab or an outside one
Pin or bushing tested on a non-fit diameterConfirm the lab corrected for the convex surface (ASTM E18)
Thin or small partConfirm the thickness was enough for the scale used (ASTM E18)

About those last two rows: ASTM E18 says the Rockwell test is considered satisfactory for acceptance testing of commercial shipments and has been used extensively that way. But the standard also includes annexes with guidelines on the minimum thickness of the test piece and with corrections for tests on convex cylindrical surfaces, which is exactly the case of a pin or the outside of a bushing. You don't need the values in those annexes; you need the lab to apply them and the certificate to say where and on what surface it tested.

If the part doesn't comply: don't install it, segregate and tag it, and ask the supplier for a test in the specified scale and the cause. With the line down, the pressure to install it anyway is huge; that's why the callout and the evidence should be settled at the quote, as explained in what to send for a same-day quote on an urgent spare part.

Receiving flow to verify a part's hardness: certificate with measured hardness, same scale as the drawing, test location and measured case depth where it applies, before accepting and filing the certificate with the order

Illustration: Radii conceptual diagram of the receiving flow, with references to ASTM E140, ASTM E18 and ISO 18203. Acceptance criteria and sampling are set by your quality system.

7. When NOT to call out hardness, and how Radii handles it

A hardness callout has a cost: a heat treatment, sometimes grinding afterward to finish the final dimensions, a certificate and a test. If the part doesn't work against wear, contact or localized load (a cover, a bracket, a mounting plate that only holds something), a hardness callout makes the part more expensive and adds nothing. Call out hardness where there's a functional reason, and write it complete. Where there isn't, leave it off.

At Radii, the hardness callout and the evidence you need go into the quote request, together with the drawing: that way the quote starts from what you actually need, and the evidence doesn't show up as a new cost at receiving; the heat-treat certificate comes from whoever performs the heat treatment. The capabilities that count here are 3-, 4- and 5-axis CNC milling and turning; grinding, wire EDM and honing as secondary operations (grinding is what leaves the final dimension after hardening); and CMM inspection with dimensional reports and digital traceability certificates. The shop network is audited for ISO 9001 and AS9100 compliance, and Radii manufactures under IATF 16949 systems (details on certifications).

Frequently Asked Questions

What hardness scale should I put on the drawing of a hardened spare part?

The scale the part will be tested in, with its range and the test standard. As common practice, hardened steel is specified in Rockwell C (HRC); soft steel and nonferrous metals in Rockwell B; thin cases and small parts in Rockwell superficial or Vickers; and raw or annealed bar in Brinell. If in doubt, agree on the scale with the supplier before quoting, not at receiving.

Can I accept a part by converting an HB, HV or HLD value on the certificate to HRC?

Not as an acceptance criterion. ASTM E140 states that converting from one scale to another is an approximate process, because the tests don't measure the same combination of properties, and recommends avoiding the conversion of test data whenever possible. A conversion is good for an estimate; if the drawing calls for HRC, ask for a test in HRC.

Where is the hardness of a pin or a bushing tested?

Where the drawing says: on a non-functional face or on a coupon from the same lot, because the test leaves an indent. If the test is made on a convex cylindrical surface, such as a non-fit diameter of the pin, ASTM E18 includes correction guidelines for that case; the lab should apply them and the certificate should say where the test was made.

What should the hardness callout say for a surface-hardened part?

The surface hardness with its range and scale, plus the case depth and the method used to determine it. Surface hardness alone doesn't tell you how much hardened material there is underneath. ISO 18203 specifies a method for determining the thickness of layers hardened by surface hardening, case hardening or nitriding.

Do I need to retest hardness when the part arrives?

It depends on how critical the part is and on what your plant's quality system requires, since it sets the sampling. At a minimum, check that the certificate shows the measured hardness, in the drawing's scale, where it was tested and the lot. If any of that is missing or the part is critical, retest at the location on the drawing or have a lab do it.


Conclusion: if the hardness callout isn't complete, you can't claim against it

A hardness callout without a range, a scale and a test location can't be claimed against: any hardened part meets it, and the argument starts when the part has already failed. Write it complete (range, scale and standard, location, case if it applies and the evidence you expect) and accept the part with the test you asked for. Conversions are for estimating; acceptance happens in the drawing's scale.

If you're quoting a hardened spare part or tooling component, upload your drawing or CAD to Radii with the complete hardness callout and the evidence you need stated in the request.

Sources

  • ASTM International, ASTM E18-24, Standard Test Methods for Rockwell Hardness of Metallic Materials. Only the scope and the “Significance and Use” section on the standard's public page were consulted.
  • ASTM International, ASTM E140-12b(2019)e1, Standard Hardness Conversion Tables for Metals (short title). Only the scope and the “Significance and Use” section on the standard's public page were consulted.
  • ISO, ISO 18203:2026, Steel — Determination of the thickness of surface-hardened layers, edition 2 (January 2026), ISO/TC 17/SC 7. Only the public abstract was consulted.

Have a project in mind?

Optimize cycle times and costs with our manufacturing network. Receive pricing and manufacturability validation in minutes.

Certifications
Secure Data Protection
Nearshore Leader